The Comprehensive Guide to the Zirconia Bonding Protocol: APC Concept and Clinical Evidence
Master the zirconia bonding protocol. Learn the APC concept, 10-MDP chemical bonding, and decontamination steps for long-term clinical success

Zirconia Bonding Protocol: The APC Concept, Step by Step
A reliable zirconia bonding protocol follows three steps: air-particle abrasion, a primer with a phosphate monomer such as 10-MDP, and an adhesive resin cement, the sequence known as the APC concept. Below are the products used at each step, followed by the evidence and a chairside protocol for zirconia cementation.
Which Products Do You Need for Each APC Step?
The products are grouped in the order you use them: abrasion of the intaglio surface, cleaning after try-in, priming and cementation. Each primer and cement has its own instructions for use, so follow the protocol of the system you choose.
Air Abrasion of the Zirconia Intaglio: Danville 50 Micron Aluminum Oxide
Danville's 50 micron white aluminum oxide is a medical-grade alpha alumina powder for chairside microetchers and lab sandblasters. On zirconia it is the A step of the APC protocol: abrade the intaglio at low pressure until it is uniformly matte, and use it again to clean the surface after try-in. Best for: Practices that air-abrade zirconia, metal and composite restorations chairside before cementation
Post-Try-In Cleaning of Restoration Surfaces: Ivoclar Ivoclean
Ivoclean is a cleaning paste, a dispersion of metal oxide particles in water, for the extraoral cleaning of ceramic and metal restorations contaminated during try-in. It is applied to the bonding surface for 20 seconds, rinsed and dried, and the primer is then applied again. It is not for intraoral use. Best for: Cleaning zirconia and other ceramic restorations after try-in when re-abrasion is not an option.
Cleaning of Tooth and Restoration After Try-In: Kuraray Katana Cleaner
Katana Cleaner is based on a 10-MDP salt and works on both sides of the bond: zirconia, glass ceramic, resin and metal restorations, fiber posts, implant abutments and the prepared tooth. It is rubbed on for more than 10 seconds, rinsed until the color disappears and dried with mild oil-free air. Best for: Decontaminating the preparation and the restoration with one product after try-in.
Universal Restoration Primer for Zirconia and Glass Ceramics: Ivoclar Monobond Plus
Monobond Plus is a single-component universal primer, an alcohol solution of silane methacrylate, phosphoric acid methacrylate and sulfide methacrylate, so one bottle primes oxide ceramics such as zirconia, glass ceramics, metal and fiber-reinforced composite. It reacts for 60 seconds before being dispersed with a strong stream of air. Best for: Practices that bond zirconia, lithium disilicate and metal and want one primer for all of them.
Multi-Substrate Primer With MDP and Silane: GC G-Multi PRIMER
G-Multi PRIMER combines silane, MDP and MDTP in one bottle to prime zirconia, alumina, glass and hybrid ceramics, composite and metal before luting, and for intraoral or extraoral repairs. It is applied as a thin layer and air-dried, with no waiting time required by the instructions. Best for: Mixed indirect workflows and chairside repairs where the substrate changes from case to case
Dedicated Zirconia, Alumina and Metal Primer: Bisco Z-Prime Plus
Z-Prime Plus is a single-component primer that pairs MDP with a carboxylate monomer, BPDM, for zirconia, alumina, metal, composite and endodontic posts. One or two coats are applied and air-dried, and the instructions also allow priming before try-in, followed by rinsing. Best for: Clinicians who prefer a dedicated zirconia primer, separate from the tooth adhesive.
Self-Cure Adhesive Resin Cement for Opaque Zirconia: Ivoclar Multilink Automix
Multilink Automix is a self-curing luting composite with an optional light cure, used with self-etching Multilink Primer A/B on the tooth and Monobond Plus on the restoration. Because it cures without light, it suits opaque zirconia as well as metal, glass ceramic and composite restorations, and excess is tack-cured in quarter sections and removed with a scaler. Best for: Adhesive cementation of zirconia on short or tapered preparations and resin-bonded bridges.
Self-Adhesive Resin Cement for Retentive Crowns: Dentsply Sirona Calibra Universal
Calibra Universal is a dual-cure, fluoride-containing self-adhesive resin cement for ceramic, composite and metal-based crowns, bridges, inlays, onlays and posts, with no separate tooth adhesive. Excess is tack-cured for up to 5 seconds per surface and removed in the gel phase, and the restoration is pretreated as the instructions describe. Best for: Zirconia crowns on retentive preparations where a simplified self-adhesive protocol is enough.
The Foundation of the APC Concept
Zirconia is a polycrystalline ceramic with no glass phase, so the hydrofluoric acid etching and silane that work on lithium disilicate do not create a durable bond to it. The APC concept, described by Blatz and colleagues in 2016, answers this with three steps: (A) air-particle abrasion, (P) a zirconia primer and (C) an adhesive composite resin cement.
Each step solves a different part of the problem. Abrasion creates micromechanical retention and a clean, reactive surface, the primer forms a chemical bond with zirconium oxide, and the resin cement links the primed restoration to the bonded tooth. A systematic review of clinical studies on bonded zirconia restorations reached the same recommendation: 50 micron alumina at low pressure, combined with an adhesive resin that contains a phosphate monomer, under rubber dam isolation.
Phase A: Air-Particle Abrasion and Mechanical Micro-Etching
The A in the APC concept stands for air-particle abrasion of the intaglio surface. It creates micromechanical retention and raises the surface energy, so the primer and the cement can wet the zirconia.
The Physics of Sandblasting
Use 50 micron aluminum oxide at low pressure, between 1 and 2.5 bar (about 15 to 35 psi), the range recommended by the systematic review cited above. Abrade until the intaglio is uniformly matte, then remove the residual powder with oil-free air before priming.
More pressure is not better. Aggressive abrasion can trigger a phase transformation from tetragonal to monoclinic zirconia and can damage the surface, which matters most on thin margins and on high-translucency zirconia. The goal is a uniform matte surface with the least energy needed to get it.
Benefits of Mechanical Preparation
Air abrasion also cleans. After saliva contamination, re-abrading the intaglio restored bond strength better than the other cleaning methods tested in the laboratory, which is why many clinicians abrade after try-in rather than before it. Abrasion alone is not a bonding protocol, though: the clinical recommendation is to pair it with a phosphate monomer primer or adhesive.
Phase P: Chemical Priming and the Power of 10-MDP
The P step applies a primer that bonds chemically to zirconia. That bond comes from phosphate monomers, and the most studied is 10-MDP (10-methacryloyloxydecyl dihydrogen phosphate).
The Role of the 10-MDP Monomer
The phosphate end of 10-MDP bonds to the zirconium oxide on the restoration, while the methacrylate end copolymerizes with the resin cement. This is why zirconia primers, and many universal adhesives, list MDP or another phosphate monomer among their ingredients.
Some universal adhesives, such as Scotchbond Universal Plus, contain MDP and are indicated by their manufacturers as zirconia primers, so one bottle can treat both the tooth and the restoration. A dedicated primer such as Z-Prime Plus, or a multi-substrate primer such as Monobond Plus or G-Multi PRIMER, is the simpler choice when the cement system calls for one or when the same appointment includes glass ceramics or metal. For the adhesives themselves, see our guide to the best dental bonding agents.
Managing Surface Contamination and Decontamination
Try-in is the most common point of failure in a zirconia bonding protocol. Saliva and blood coat the intaglio surface within seconds, and their phosphate-containing proteins and phospholipids attach to the same zirconium oxide sites that the primer needs to reach.
Why Phosphoric Acid Fails
Phosphoric acid is the reflex choice for cleaning, but it does not decontaminate zirconia. In a systematic review and meta-analysis of laboratory studies, phosphoric acid and alcohol gave bond strengths no better than a water rinse after saliva contamination. The Monobond Plus instructions say the same: do not clean zirconia or metal with phosphoric acid.
Effective Decontamination Protocols
The same meta-analysis found that re-abrading with aluminum oxide gave the highest bond strength after contamination, and that a cleaning paste such as Ivoclean also performed better than water. Two practical sequences follow:
- With an air abrasion unit chairside or in the lab: abrade the intaglio after try-in, then prime.
- Without one: apply a cleaning paste to the restoration outside the mouth, rinse, dry and prime right away. A cleaner such as Katana Cleaner can also be used on the prepared tooth; check the indications in its instructions.
Phase C: Composite Resin Selection and Cementation
The C step, the last stage of the zirconia bonding protocol, is the resin cement. Zirconia attenuates curing light, more so in thick or opaque restorations, so choose a dual-cure or self-cure cement and do not rely on light curing alone under the restoration.
Cement Type, Film Thickness and Isolation
Adhesive resin cements used with a separate tooth adhesive give the most retention and are the choice for short or tapered preparations, resin-bonded bridges and thin restorations. Self-adhesive resin cements simplify the procedure and work well on retentive crown preparations. In both cases a low film thickness helps the restoration seat fully, and rubber dam or reliable isolation keeps the bond free of contamination during cementation.
Clinical Summary and Final Recommendations
The zirconia bonding protocol, step by step:
- Try in the restoration and check fit, contacts and occlusion.
- Clean the intaglio: re-abrade with 50 micron alumina at 1 to 2.5 bar, or use a cleaning paste outside the mouth. Do not use phosphoric acid on zirconia.
- Prime the intaglio with an MDP-containing primer, or a universal adhesive indicated for zirconia, and respect the reaction time in its instructions.
- Isolate the tooth, preferably with rubber dam, and treat it with the adhesive of the cement system.
- Cement with a dual-cure or self-cure resin cement, remove the excess at the gel stage and complete the light cure from every surface.
- Check the occlusion and floss the contacts to remove residual cement.
Zirconia Bonding: Frequently Asked Questions
What is the APC concept for zirconia?
APC stands for air-particle abrasion, primer and composite resin cement. It is a three-step zirconia bonding protocol: abrade the intaglio with 50 micron alumina at low pressure, apply a phosphate monomer primer such as 10-MDP, and cement with an adhesive resin cement.
Can you use phosphoric acid to clean zirconia?
No. Phosphoric acid does not remove salivary contamination from zirconia, and in laboratory testing it performed no better than water. Re-abrasion, or a cleaning paste designed for restorations, is the effective option.
Do you need a separate zirconia primer?
Not always. Many universal adhesives contain MDP and are indicated as zirconia primers. A dedicated primer is useful when the cement system requires it, or when you bond zirconia, glass ceramics and metal in the same workflow.
Is self-adhesive resin cement enough for zirconia crowns?
On retentive crown preparations, yes: self-adhesive resin cements are widely used for zirconia crowns. Short or tapered preparations, resin-bonded bridges and veneers need the full zirconia bonding protocol with an adhesive resin cement.
Zirconia Bonding Materials and Alara: Get the Best Deals from Trusted Suppliers
Primers, cleaners and resin cements are small items with wide price differences between vendors. Alara compares real-time offers on every product in this guide, from Ivoclean and Monobond Plus to Multilink Automix, across 15+ verified vendors.
Ready to Start Saving on Dental Supplies?
Join hundreds of dental practices already using ALARA to compare prices and streamline their supply ordering.
References
- Quigley NP, Loo DSS, Choy C, Ha WN. Clinical efficacy of methods for bonding to zirconia: A systematic review. J Prosthet Dent. 2021;125(2):231-240. PMID: 32115220. DOI: 10.1016/j.prosdent.2019.12.017
- Silva NRD, Araujo GM, Vila-Nova TEL, Bezerra MGPG, Calderon PDS, Ozcan M, Souza ROAE. Which zirconia surface-cleaning strategy improves adhesion of resin composite cement after saliva contamination? A systematic review and meta-analysis. J Adhes Dent. 2022;24:175-186. PMID: 35416445. DOI: 10.3290/j.jad.b2916437
More Articles

Best Prophy Paste for Dental Hygiene Appointments: Grit, Fluoride and Format
Prophy paste by grit, RDA, fluoride and format: selective polishing, heavy stain, sensitive teeth, restorations, gluten-free pastes, cups and jars.
November 16, 2026

Nitrile vs Latex Gloves: What Dental Practices Should Stock
Nitrile, latex and chloroprene dental exam gloves compared on allergy risk, puncture resistance, fit and cost per box, with the criteria for setting a practice standard
August 19, 2026

Root Canal Sealers Compared
Root canal sealer classes compared: epoxy resin, calcium silicate, and zinc oxide eugenol, matched to obturation technique and handling
August 18, 2026